Anti settling agents only focus on preventing static settling, and are not directly responsible for good dispersion and agitation; Many times, anti settling agents are added, but the precipitation is not easy to form hard lumps. However, the system itself has low viscosity, pigment aggregation, and no thixotropy, making it difficult to stir, unable to stir, and unable to open.
Below is a summary of the reasons and corresponding solutions (applicable to both water-based and solvent based coating systems, distinguishing common anti settling agents such as HEUR, bentonite, fumed silica, and polyamide wax):
1、 The most common types of reasons
1. The anti settling agent has not been truly activated/effective
Polyamide wax (commonly used solvent based): It must be activated by heating (generally 40-60 ℃, different grades vary), and dispersed at high speed for a period of time; When added directly at low temperature, the wax does not form a three-dimensional network structure, only powder particles, without thixotropy, and cannot suspend or reduce agglomeration. It is just mixed inside, and the pigment lumps still remain dead and difficult to stir.
Organic bentonite: requires polar activators (ethanol/acetone/propylene glycol, etc.) and high shear. If not fully activated, it will agglomerate into dry powder and become impurities, making it more difficult to stir.
HEUR polyurethane thickening and anti settling (most commonly used water-based): sensitive to pH, cosolvents, and surfactants; If the pH is not correct and there is an excess of anionic dispersants in the system, it will antagonize HEUR and cause thixotropy, resulting in only medium to high viscosity without the thixotropy of “becoming thinner when stirred and thicker when stopped”.
✅ Phenomenon: After standing still for a period of time, the pigment will layer, sink to the bottom, or the viscosity may appear high, but there is no smooth or thixotropic texture, like a paste that is “dead thick” and difficult to stir.
2. Mismatch and antagonism between anti settling agents and dispersants
Anti settling agents are used to establish a mesh structure to support pigments; Dispersants are adsorbed on the surface of pigments to separate and aggregate.
Adding too many anionic dispersants can seize the surface of the pigment and damage the bentonite HEUR、 Network of magnesium aluminum silicate;
Some polymer dispersants may encapsulate anti settling agent particles, inhibiting network formation; The aggregates have not been opened, and the anti settling agent supports pigment aggregates, not native particles. No matter how you stir them, they will still stir the aggregates, which feels heavy and difficult to disperse.
Key sequence: First add dispersant → high-speed dispersion to grind the pigment sand to fineness → then add anti settling agent; Many people add anti settling agents before adding color powder, and the pigment is directly wrapped in the thixotropic network, which cannot be opened and is extremely difficult to mix.
3. Only anti sinking measures were added, without sufficient [thixotropic structure], resulting in ‘Newtonian viscosity’ rather than thixotropic viscosity
The two viscosities are completely different:
Newtonian thickening: simply increasing viscosity, with almost no decrease in viscosity during stirring → the thicker the viscosity, the harder it is to stir, and it is very heavy and laborious to stir
Thixotropic anti settling: Hold the pigment with high viscosity at rest, and the viscosity quickly decreases when sheared (becomes thinner when sheared) → Easy to stir, and when stopped, the viscosity returns to prevent settling
Differentiation test: Pick a small amount of material and place it in a beaker. Insert the glass rod still and there is high resistance. Stir it quickly. If it is still thick and does not flow, it will cause poor thixotropy.
4. Problems with the pigment itself
Carbon black, organic red/purple, ultrafine titanium dioxide, iron oxide, with extremely strong primary agglomeration; If there is no sand grinding and only relies on the dispersion plate for stirring, with the addition of dispersants and anti settling agents, the aggregates cannot be broken, resulting in hard particle clusters that are difficult to stir apart;
The oil absorption value of the pigment is too high, which can absorb the resin/solvent in the system, resulting in local dry material lumps, and the anti settling mesh cannot hold the hard agglomeration.
5. Incorrect timing and method of addition
1. The anti settling agent is directly added to the pigment slurry as a dry powder: the dry powder absorbs water/solvent and forms clumps, turning into small white lumps that wrap around the pigment;
2. Insufficient high-speed dispersing speed and dispersing disc line speed;
3. After adding anti settling materials, immediately discharge the material without any static curing time (bentonite, wax slurry, magnesium aluminum silicate generally require 20 minutes to several hours of curing, and the network slowly grows out);
4. The solid content of the system is too high, and the pigment volume concentration of PVC is close to/exceeds the critical CPVC. The flowability of the slurry itself is extremely poor, and the anti settling agent will only add insult to injury.
6. Interference from other additives
Excessive defoamers, leveling agents (especially organosilicon), and substrate wetting agents can damage the thixotropic network with many surfactants; Solvent type: Too much strong solvent can cause swelling/damage to the network crystal structure of polyamide wax, resulting in ineffective anti settling and pigment aggregation and floating/sinking to the bottom.
2、 Quick troubleshooting sequence
1. Feeding sequence: resin → solvent/water → dispersant → pigment → high-speed dispersion+sanding until the fineness is qualified → finally add pre activated anti settling agent, leveling defoamer ✅ (Do not reverse)
2. Confirm whether the anti settling agent is activated: whether the polyamide wax slurry has insulation activation, whether the bentonite has added activator, and whether HEUR is slowly added after dilution
3. Look at thixotropy: Make a thixotropy index (viscosity ratio of 6rpm/60rpm), low thixotropy index=shear thinning, difficult to stir
4. Reduce the dispersant a bit, or switch to a dispersant compatible with anti settling (such as using a non-ionic dispersant combined with HEUR for greater stability)
5. Check the fineness: Use a fineness meter to check for a large number of agglomerated particles. If there are particles, it means they are not dispersed properly, not due to sedimentation prevention issues
3、 Targeted adjustment plan
Solvent based (polyamide wax): Use pre activated wax slurry, disperse at 60 ℃ for 15-20 minutes, and do not add dry powder; Paired with a small amount of fumed silica to assist in thixotropy
Water based (HEUR system): Replace with high contact HEUR, do not use ordinary thickening type; Control the dosage of anionic dispersants, and it is necessary to use magnesium aluminum silicate to synergistically prevent sedimentation and reduce dead thickness
· Bentonite system: must pre gel, sufficient polar activator, high shear, do not directly put dry powder
Difficult dispersion of pigments: Increase the sanding time, add appropriate wetting and dispersing agents, and do not expect anti settling agents to open the pigment clusters