Leveling agents regulate surface tension and cannot elongate the leveling window; Choosing the wrong, adding too much, not matching the system, and fighting with additives can create new surface tension gradients (Marangoni convection), forming wavy orange peel.

1. Excessive leveling agent

Organic silicone leveling agents are particularly noticeable: when applied in appropriate amounts, evenly spread on the surface and smooth out tension differences; After exceeding the limit, the distribution is uneven, and the local surface tension fluctuates between high and low. The internal convection of the wet film forms fine ripple orange peel, accompanied by flower and fog shadows.

Conventional recommendation for silicon-based materials: 0.1-0.3%, and many systems are prone to problems if they exceed 0.4%.

2. Selection error, incompatible with resin/system

Acrylic leveling agent: Good compatibility, mainly used to eliminate brush marks, roll coat orange peel, and reduce weak surface tension; If you were supposed to compress the hole, using it alone won’t work;

Polydimethylsiloxane (ordinary silicone oil): It has strong tension reduction and poor compatibility. Many baking paints, PU, and UV systems have ripples and orange peel when added;

Choosing the wrong type of modification: for example, using poorly compatible silicon for quick drying solvent type, or using fluorocarbon leveling agents with strong migration for UV system;

Mechanism: Insufficient compatibility → The leveling agent undergoes phase separation and local enrichment during film formation, spontaneously forming convective patterns that appear to be orange peel.

3. Compatibility conflict of additives

Defoamers, wetting agents, dispersants, lubricants, and leveling agents interfere with each other:

The defoamer itself is a low surface tension substance, and with the addition of silicon leveling agent and multiple surfactants, the tension is repeatedly disturbed;

Many people desperately replenish leveling agents in order to save the shrinkage cavity, but as a result, the shrinkage cavity is pressed down and convective ripples emerge.

4. The leveling window itself is too short, and leveling agents cannot save it

Orange peel essence: before the wet film flattens the spray ripples, the viscosity will rapidly rise and gel/surface will dry. Leveling agent does not change the solvent evaporation rate and curing rate:

The diluent evaporates too quickly, the flash drying is too short, and the baking temperature rises sharply;

UV: High concentration of photoinitiator and excessive light intensity can instantly cure the surface of the cover;

Dual component: high proportion of curing agent and high ambient temperature; The surface layer first forms a crust, while the lower layer is still flowing → the surface layer is pulled out with orange peel; At this point, adding more leveling agents is ineffective and may even exacerbate convection.

5. Secondary issues caused by pigments/fillers, viscosity, and film thickness

High oil absorbing pigments and ultrafine fillers are abundant, and the system has high viscosity and elasticity; Leveling agents only alter interfacial tension and cannot reduce bulk viscosity. After the leveling agent migrates to the surface, the viscosity difference between the surface and the bulk increases, making it more prone to surface slip ripples.

Quick troubleshooting sequence

1. First, reduce the amount of leveling agent added and conduct a halving test (priority, often 0.05-0.15% is sufficient);

2. Distinguishing types: Silicones are prone to convective orange peel; First switch to acrylic leveling agent for comparison;

3. Solvent/volatile equilibrium: Add a small amount of high boiling slow drying solvent and elongate the leveling window;

4. Auxiliary isolation: Do not add defoamers and high added silicon leveling agents together;

5. Exclude construction: poor atomization, uneven film thickness, high wind speed, and substrate contamination;

6. UV system: Reduce the curing speed of the surface layer beyond oxygen blocking, avoiding premature film locking.

Simply distinguish between two types of orange peels

Orange peel caused by leveling agents: fine ripples, accompanied by floral patterns, bright and dark stripes when viewed from the side, moist film appears moist, and wrinkles appear after curing;

Fast evaporation/solidification of orange peel: Large wavy orange peel, with retained spray texture and no obvious flower development.