news

The essence of baked brittle fracture is that the internal cohesion of the coating is greater than the fracture toughness, and the stress exceeds the limit that the film layer can withstand; Divided into two categories: insufficient toughness of the formula itself (intrinsic brittleness)+internal stress caused by baking process (stress-induced cracking), the two often overlap. Combining what you have been looking at earlier: resin polarity, acid value, crosslinking, pigment crystal form, and compatibility of additives, many pits are interconnected.

First, distinguish the two most common appearances and quickly locate them: 1) cracking only after cooling after being taken out of the furnace (cooling cracks, accounting for 80%): cooling shrinkage stress is the main cause; 2) Direct cracking of high-temperature insulation section: high-temperature thermal degradation, excessive cross-linking, premature hardening and solidification.

1、 Internal factors in the formula

1. High cross-linking density

Too many cross-linking points and too tight cross-linking network result in the loss of slip ability of molecular chain segments, and the toughness directly returns to zero, becoming a rigid brittle network.

Typical scenarios: high acid resin+excessive epoxy/aziridine/HDI curing agent, excessive addition of hydroxyl resin curing agent, high baking temperature/long time, excessive cross-linking

Features: High hardness, decent adhesion when scratched, but brittle fracture directly due to bending, impact, and thermal cycling; The thicker the film, the easier it is to crack

Related to your previous knowledge point: High acid resin is based on carboxyl groups, with multiple cross-linking sites, making it very easy to become brittle due to excessive cross-linking. Many people only pursue water resistance, and adding curing agents can directly make it brittle. Comparison: Suitable crosslinking – the crosslinked network has a small number of flexible segments that can absorb stress; The cross-linking is too high, the chain segments are locked, and there is no deformation buffering.

2. The main chain structure of the resin itself lacks flexible segments

The proportion of rigid skeleton is too high: a large number of benzene rings, aromatic rings, aliphatic rings, and high Tg monomers, lacking long-chain alkyl groups, polyethers, and flexible units of fatty chains

Tg is much higher than room temperature: after film formation, it is already a glassy hard and brittle material

Example: Pure styrene acrylic acid, high aromatic epoxy, partially high Tg polyester, without flexible monomer modification, easily brittle

3. Excessive pigment/filler filling, hard powder, poor particle size matching

Powder is a rigid particle, filled to a concentration near/exceeding the critical volume concentration of CPVC:

Resin has less continuous phase transition, and the powder is bonded by a thin layer of resin, which is insufficient to cushion stress

High hardness and oil absorbing fillers such as barium sulfate, talc powder, and silicon dioxide are added in high quantities and exhibit significant brittleness;

The crystal form/surface treatment of pigments also has an impact: poor surface coating of pigments and weak resin interface become the starting point of cracks;

Phenomenon: The film is fine, but the thick coating immediately cracks; Reducing the amount of pigment and filler, and changing to a lower oil absorbing powder have significantly improved the situation.

4. Phase separation and interface defects caused by additives

Low polarity additives added to high polarity and high acid baking paint systems have poor compatibility and precipitate within the film to form small defects and weak interfaces

The micro phase separation zone is the source of crack initiation

Excessive addition of wax powder can also reduce the cohesive toughness of the coating, make it brittle, and decrease its adhesion

5. Residual small molecules and volatile matter

The baking curve is incorrect, and the solvent is trapped in the cross-linked network: at high temperatures, the internal solvent vaporizes and expands, producing pores and microcracks; After cooling, micropores are weak points that can crack upon contact. Water based baking paint is particularly prone to problems such as slow evaporation of water and amine neutralizing agents, rapid heating, surface coating, and inability to come out from the inside.

2、 Stress issues caused by baking process

Source of thermal stress: mismatched coefficient of thermal expansion of coating and substrate+too fast heating/cooling rate

1. Rapid heating: The surface layer first solidifies and forms a crust, while the lower layer’s solvent and water continue to evaporate, resulting in internal compressive stress;

2. Too fast cooling rate: The high-temperature film rapidly cools down, and the coating shrinkage rate is greater than the substrate shrinkage rate, generating huge tensile stress. Once the tensile stress exceeds the coating fracture toughness, it will directly crack;

The difference in expansion coefficient between metal substrates and organic coatings is very large, and this effect is amplified on thick film and high Tg baking paints.

1. Baking temperature exceeds the resin thermal decomposition temperature: resin chain segments undergo thermal degradation, chain breakage, oxidation, and the polymer loses elasticity, directly turning into powder and becoming brittle

Differentiation: Degradable brittleness – the coating turns yellow, powdery, and shatters easily after baking; Simple stress brittleness, normal color, only cracks after bending after cooling.

Addendum: Amplification effect of film thickness

The same formula and process: the thicker the film, the greater the total shrinkage, the greater the stress, and the easier it is to crack. Many baking paint indicators: the recommended upper limit of film thickness is the critical thickness for brittle fracture.

3、 Substrate factors

1. The substrate itself has high rigidity and invisible space: thick steel plate, hard aluminum, glass, compared to soft aluminum plate and galvanized plate; Soft substrates can deform and share stress, while hard substrates are fully stressed by the coating;

2. Primer problem: The primer is too hard, the interface between primer and topcoat is weak, and stress is concentrated at the topcoat/primer interface, manifested as topcoat cracking, and even interlayer peeling cracking;

3. Surface contamination of the substrate, local poor adhesion, and localized stress concentration leading to cracking.

4、 Quick diagnosis and troubleshooting process

1. First, check the timing of cracking ✅  Cracking, yellowing and powdering during the high-temperature insulation stage → Priority: high temperature, thermal degradation, excessive cross-linking ✅  Slowly crack after cooling for a few minutes → Priority: cooling too fast, thermal shrinkage stress, Tg too high ✅  It only cracks after bending and impact, and cannot be opened due to insufficient toughness, high cross-linking, and excessive filling ✅  Thick film cracking, thin film not cracking → stress+CPVC filling problem

2. Simple control experiment for comparison

Reduce the proportion of curing agent during baking: no cracking=excessive cross-linking

Reduce film thickness test: no cracking=stress dominant

Step cooling (slow cooling inside the oven after baking): no cracking=cooling rate too fast

Reduce talc/barium sulfate fillers: Improvement=filling brittleness

Reduce peak baking temperature, extend insulation, slow heating: Improvement=solvent coating/surface cover

5、 Formula&Process Improvement Direction

Formula end

1. Control crosslinking density: reduce the equivalent of curing agent; Introducing flexible monomers/polyols and long-chain fatty segments to reduce the bulk Tg and increase the elongation at break;

2. Color fillers: reduced to below CPVC; Prioritize low oil absorbing fillers; Good dispersion of powder to avoid agglomeration;

3. Additives: Match polarity to avoid excessive addition of incompatible silicon additives; Reduce wax powder;

4. Resin selection: Do not blindly pursue high acidity, high hardness, and high water resistance. Hardness and toughness are a pair of balancing indicators.

Process end

1. Segmented heating: The pre drying area evaporates slowly to prevent the cover from drying and to drive away solvents/water;

2. Do not overheat and strictly follow the curing window;

3. The cooling section cannot be rapidly cooled, and gradient cooling is required;

4. Control the upper limit of dry film thickness.


Post time: Nov-27-2026