news

The essence of dispersion is to break down carbon black aggregates and stabilize the separation of primary particles; Lack of dispersion → low blackness and brownish yellow color; Excessive dispersion (over grinding) → Blackness drop, weak blue phase transition, and even graying; The dispersion system, additives, and shearing method directly determine the final color (blue phase/brown phase).

The finer the primary particles of carbon black itself, the stronger the intrinsic blue phase; But whether it can be reflected depends entirely on the dispersion.

1、 First, clarify two concepts

1. Blackness (coloring power/carbon black blackness): Under the same amount of addition, the lower the reflected light of the paint film, the higher the blackness. Carbon black aggregates are large particles that scatter visible light, resulting in whitening, graying, and poor blackness.

2. Undertone base color: Carbon black base color is divided into blue phase (cool black) and brown phase (warm black). Fine grained high structure carbon black naturally has a bluish phase; Coarse particle size, low structure, and brownish phase. Blue phase is not a single attribute of carbon black, dispersion can change the appearance of the base color.

2、 The impact of each variable in the dispersion process on each item

1. Pre dispersion

Pre mixing purpose: Wet the surface of carbon black agglomeration, replace air with resin/solvent/water, and avoid dry agglomeration of dry carbon black.

Insufficient wetting: The carbon black powder agglomerates are aerated, making it difficult to open during later grinding. The finished product has low blackness, obvious brown phase, and stuffiness; Agglomeration particles cause bright spots and particle dots.

Excessive wetting (long-term low-speed pre stirring): Some carbon black floats and coagulates prematurely, especially in aqueous systems, with unstable blue phase and large batch color difference.

Key: Wetting/dispersing agents must be added before adding carbon black, first wetting the carrier, and then adding carbon black.

2. Grinding shear strength

① Insufficient cutting

Only a portion of the agglomerates are broken, leaving a large amount of residual agglomerates

Blackness: Low, appearing grayish black

Blue phase: Blue phase cannot be produced, leaning towards a brownish yellow background. Principle: Large aggregates preferentially scatter short wave blue light, causing blue light to be scattered and lost, leaving only brown tones visually.

② Cut appropriately (optimal dispersion range: agglomeration opens, native particles do not break)

Carbon black is uniformly and stably dispersed into primary particles/small aggregates

Blackness: reaching peak value

Blue phase: fully released, cool toned blue black, is the target state.

③ Excessive cutting

⚠️  Key point: The primary particles of carbon black will not be broken, but the structure of carbon black will be destroyed, dispersants will desorb, and secondary flocculation will occur

Blackness: On the contrary, it has decreased (often referred to as “worn out” in the industry)

Blue phase: The blue phase decays from cool black to gray black, brown black; Gloss decreases synchronously. mechanism:

1. The chain like structure of high structure carbon black is broken by external force, causing a decrease in structure, coloring power, and blue phase;

2. Dispersants desorb from the surface of carbon black, causing particles to re aggregate and form tiny flocs;

3. When the system heats up, the compatibility between the dispersant and the resin changes, causing the color paste to thicken.

Water based carbon black paste is very prone to the problem of blue phase running away due to excessive grinding.

3. Grinding media

Large beads: Strong impact force, suitable for opening large pieces for aggregation; But poor dispersion and insufficient blue phase;

Small beads (0.3-0.6mm): finely cut, easier to release blue phase, higher blackness; But the small beads have a high energy density and are easily over worn;

Excessive filling rate: rapid temperature rise, continuous shear overload, and increased risk of blue phase loss.

4. Selection and dosage of dispersant

The same carbon black, changing the dispersant, the blue phase changes directly:

Anionic polymer dispersants (many acrylic acids): easier to produce blue phase black;

Partial low molecular weight wetting and dispersing agents: easy to produce brown phase black;

Insufficient addition amount: unstable dispersion, flocculation, brown phase;

Addition amount supersaturation: Free dispersants form microphase separation in the paint film, increase light scattering, decrease blackness, blue phase graying, and floating color.

If you choose the wrong dispersant for the same carbon black, no matter how hard you grind it, you won’t be able to produce a blue phase.

5. System pH and temperature

Water based carbon black:

The pH deviates from the optimal stable range of the dispersant → the particle zeta potential decreases, slowly floccules, and after storage, the blue phase drifts towards brown;

Grinding temperature is too high: the dispersant chain segment breaks, the adsorption layer desorbs, and the blue phase gradually disappears in the later stage of grinding.

6. Dispersion order

Wrong order: Resin+carbon black first, then add dispersant → The surface of the carbon black has already been occupied by the resin, and the dispersant cannot adsorb, resulting in poor dispersion and poor brown phase and blackness. Correct order: Carrier (water/solvent) → Dispersant → Wetting agent → Defoamer → Carbon black → Pre mixed wetting → Grinding.

3、 A very important phenomenon: under the same blackness, there is a difference in the blue phase

Many people mistakenly believe that high blackness equals good blueness, but this is not true:

Scenario A: Well dispersed high structure fine carbon black: high blackness+blue phase background color (cold black)

Scenario B: Insufficient dispersion and slight coagulation of carbon black: By increasing the addition amount, the blackness is increased. The base color is brown black, which looks similar to the blackness to the naked eye, but the base color is completely different. The color difference is very obvious after spraying and overlapping.

4、 Practical judgment criteria

1. Sampling with grinding time: measuring blackness and color difference (L * a * b *)

B value: Yellow index, * * the lower the b value (negative)=the stronger the blue phase; B * positive number biased towards large=biased towards brownish yellow**

Rule: During the grinding process, b first decreases (the blue phase comes out), then continues to grind after reaching the lowest point, and b rises (the blue phase runs away and begins to turn yellow brown). This lowest point is the optimal grinding endpoint.

2. Fineness board (Hegemann) can only see large particles, with qualified fineness ≠ blue phase in place! Many carbon black particles with a fineness of less than 10 μ m still have high b *, which is typical: agglomeration and fragmentation, but insufficient adsorption of dispersants and micro flocculation.

5、 Simple process optimization direction

1. Prioritize the use of polymer dispersants suitable for the carbon black, perform adsorption titration, and determine the optimal addition amount;

2. Pre mix thoroughly and wet, do not directly feed dry carbon black into the sand mill;

3. Choose suitable small zirconium beads, take time gradient sampling, and find the lowest point of b * as the grinding endpoint. Do not fix the grinding duration;

4. Control the temperature of the grinding material, and try to keep the aqueous system below 45 ℃ as much as possible;

5. After dispersion is completed, do not continue high shear stirring (high-speed stirring during the paint mixing stage can also damage the dispersion of carbon black and cause the blue phase to turn brown).


Post time: Nov-19-2026