news

The essence of plumpness: After the paint film dries, it forms a full, warm, and three-dimensional feeling with thickness, not just a simple dry film thickness; The core is the volume retention rate from wet film to dry film, leveling, thixotropy, extinction/filler combination, and film continuity.

Misconception: Only increasing the thickness can lead to sagging, wrinkling, and pinholes; There are two types of fullness: visual fullness (optical)+physical fullness (volume)

1、 Resin system

1. Glass transition temperature Tg of film-forming material and minimum film-forming temperature MFFT

Low Tg of resin: The film is soft and prone to collapse, with a thick wet film that collapses after drying, resulting in flattened and poorly plump appearance;

High Tg of resin: good film-forming rigidity, not easy to collapse, high volume retention, good fullness; But if it is too high, it is easy to crack, brittle, and difficult to level;   ✅  Control idea: the main resin is selected as the high Tg main lotion/acrylic acid/polyester, with a small amount of low Tg toughening resin to help leveling; The MFFT control of the water-based system is slightly lower than the construction temperature to ensure continuous film formation without collapsing.

2. Resin solid content, molecular weight, viscosity

High solid content resin: Under the same construction viscosity, the proportion of solid phase in the wet film is high, the volatile matter is low, the volume shrinkage rate is low, and it is better to be full and natural;

High molecular weight: viscosity surges, thin wet film during construction, and uneven flow; The molecular weight is too low, and it is prone to collapse after film formation;

3. Reference for resin type comparison

Hydroxyacrylic acid and saturated polyester: excellent fullness;

· Styrene acrylic lotion: high cost performance, general fullness; Silicon propylene>ordinary styrene propylene;

· Pure acrylic lotion: it can be adjusted well and plump, and has high requirements for auxiliary matching;

UV resin: almost non-volatile curing, shrinkage comes from double bond polymerization, shrinkage rate and functionality are related, high functional UV shrinkage is large and easy to deflate; Low functional, high volume monomers, and acrylic oligomers enhance fullness.

2、 Color filling system

With the same dry film thickness and different filler combinations, there is a huge difference in the visual fullness

1. PVC is the core indicator

Below CPVC (critical pigment volume concentration): The resin continuously wraps particles, resulting in a continuous and transparent paint film that is full and warm;

Approaching/exceeding CPVC: The resin is not sufficient to wrap the powder, with many pores, and the dry film appears weak, dry, powdery, and plummeting;   ✅  The topcoat generally controls PVC to be much lower than CPVC; Matte paint should not blindly increase the extinction powder. Adding too much extinction powder will damage the continuous resin phase and significantly reduce the fullness.

2. Packing selection

Low oil absorbing fillers (heavy calcium, barium sulfate): less absorbent resin, less resin consumption in the same amount, more excess resin, and a full paint film;

High oil absorbing fillers (light calcium, kaolin, gas-phase white carbon black): a large amount of adsorption resin squeezes the film-forming resin, making it easy to dry and thin;

Extinguishing powder: porous structure, high oil absorption, stronger extinction, more difficult to achieve fullness; Prioritize selecting low oil absorption matting powder;

Aluminum powder and pearl powder: The directional arrangement of flake pigments will “cover” the three-dimensional effect, and the fullness of metallic paint depends on the compensation of resin and wet film thickness.

3. The combination of coarse and fine particles results in denser packing and reduced voids; Single fine powder has a large specific surface area, high oil absorption, and is prone to collapse.

3、 Additive regulation (rheology, leveling, film-forming additives, directly affecting wet film retention ability)

1. Rheological additives (thixotropic system: anti sagging+moisturizing film thickness, balancing a pair of contradictions)

The fullness requires the wet film to be able to stand still after spraying, without quickly flowing off, and at the same time, it should be able to level moderately

HEUR polyurethane thickening (water-based): good leveling, transparent paint film, and friendly to fullness; Disadvantages: high addition and easy to hang; Suitable for topcoat;

HASE alkali swelling thickening: Strong thixotropy, good anti sagging, but prone to wire drawing, poor leveling, orange peel on the surface of the paint film, poor visual fullness; Generally used in combination;

Solvent based: polyamide wax, hydrogenated castor oil, gas-phase silica; Wax paste has strong thixotropy, adding too much will cause fogging and reduce transparency and fullness;   ✅  Optimal rheological structure: weak thixotropic system – viscosity decreases under spray shear, leveling and spreading; After the shear disappears, the viscosity quickly increases, locking in the thickness of the wet film and preventing it from flowing downwards. Too strong thixotropy: orange peel; Too weak thixotropy: sagging, loss of wet film, thinning.

2. Film forming aids/slow drying solvents (solvent evaporation gradient)

The matching of evaporation speed is the key point of fullness and invisibility

Quick drying: The surface quickly forms a crust, the internal solvent cannot escape, the surface locks in, the internal shrinks, and is prone to shrinkage, wrinkling, and film collapse; Looking thin;

Slow drying: Wet film with low viscosity for a long time, continuous sagging and leveling, and loss of film thickness;   ✅  Solution: Gradient evaporation, moderate evaporation in the initial stage, and retention of a small amount of slow drying components in the later stage, allowing the paint film to shrink synchronously and slowly, forming a uniform film without pre covering the surface layer; Water based: film-forming agents should not be used in large quantities with high boiling points at once, and should be paired with alcohol ether gradients; Solvent type: A combination of fast and slow solvents to avoid using a single ultra-high boiling point solvent.

3. Leveling agent, defoamer

Leveling agent: moderately added to eliminate orange peel, make the gloss uniform, and enhance visual fullness; Excessive migration, shrinkage, and oil level;

Defoamer: Residual bubbles will form voids inside the paint film, which will become concave and pitted after drying, severely damaging the fullness; Microbubbles must be controlled.

4、 Construction end control

1. Wet film thickness takes priority, with dry film thickness as a supplement. The fullness is determined by the combination of wet film thickness and shrinkage rate; Shrinkage rate=(wet film thickness – dry film thickness)/wet film thickness Example: For high shrinkage coatings, the wet film thickness is 100 μ m, and the dry film thickness is only 35 μ m; Low shrinkage high solid moisture film 80 μ m, dry film 60 μ m, the latter being fuller and better.

2. Spray parameters

Atomization pressure: If the pressure is too high, the paint mist will be fine and the wet film will be thin; Low pressure, high paint output, and thick wet film; But the pressure is too low, resulting in poor atomization and orange peel;

Gun speed and overlap rate: slow gun speed and high overlap → wet film thickness;

Dilution ratio: The more diluted, the lower the solid content, the greater the shrinkage, and the decrease in fullness; Try to dilute the topcoat as little as possible;

3. Interval between layers (flash drying time) Wet touch wet spraying: If the flash drying is too short, the lower solvent will impact the upper layer, causing bottom biting and sagging; Flashing dry for too long, the first layer has already dried hard, and the second layer cannot be integrated, layered, and the three-dimensional sense is fragmented, with poor fullness;

4. Baking conditions (baking paint): Heating up too quickly: rapid surface solidification, internal solvent expansion, later collapse, pinholes;   ✅  Low temperature pre drying (leveling section) → further heating and curing: give enough leveling and relaxation time, then crosslink and shape to lock in a full form.

5、 Special instructions for UV system

UV has almost no solvent evaporation, and the shrinkage comes from the volume shrinkage of photopolymerization

High functional monomers/resins: high cross-linking density, large shrinkage, inward shrinkage of paint film, easy to deflate;

Regulation: Reduce the average functionality of the system; Introducing cyclic monomers, epoxy acrylic acid, and high volume low shrinkage monomers; Paired with a small amount of flexible oligomers; Control the curing energy and avoid overexposure;

UV fullness difficulty: curing too fast, very short leveling window; It needs to be matched with low viscosity, suitable thixotropy, and given a few seconds of leveling time before curing.

6、 Quickly optimize the troubleshooting sequence

Insufficient fullness, investigate in this order:

1. Tested whether the PVC is too high and whether there is an increase in matting powder/high oil absorbing fillers → Prioritize reducing PVC and replacing with low oil absorbing fillers

2. Is the resin solid content too low and has too much shrinkage? Increase the solid content of the system

3. Rheology: Is it because the thixotropy is too weak and the orange peel has flowed away? Adjust the thickener ratio to achieve weak thixotropy

4. Solvent/film-forming agent: Does fast drying cause surface drying, crust formation, and film collapse? → Compound slow drying components to elongate the leveling window

5. Construction: excessive dilution, too thin wet film spraying, incorrect flash drying time

6. Bubbles and pinholes in the paint film

7、 Reminder of common reverse side effects

Blindly increasing the wet film thickness: sagging, flow marks, bubbles, undercutting, cracking;

A large amount of slow drying solvents: rebound, poor stain resistance, slow drying;

Reduce the excessive addition of resin to PVC: cost increase, loss of gloss, and decrease in hardness;

To achieve fullness in matte paint, it is necessary to accept slightly higher gloss or use low oil absorbing matte powder. It is not possible to pursue extremely low gloss while achieving ultimate fullness, as the two are naturally balanced.


Post time: Nov-17-2026