1、 Substrate processing
1. Steel priority sandblasting/shot blasting: Sa2.5 grade, roughness 40-70 μ m; Due to limited conditions, power tools can be used to polish to St3 level, but manual rust removal and rust prevention are much less effective
2. Oil stains and grease should be cleaned with solvents first; Polish and smooth welding slag, spatter, and burrs; Salt content should be controlled (≤ 50mg/m ²), with a focus on controlling salt spray environments
3. The surface is dry, free of floating rust and dust; The substrate temperature should be above 3 ℃ above the dew point to prevent condensation, flash rust, whitening, and pinholes
4. Galvanized and aluminum plates: light polishing/phosphating treatment, direct spraying is prone to paint peeling; The old coating needs to be polished and brushed, and all hollows and peeling should be removed
2、 Proportioning, maturation, and activation period
1. Strictly follow the TDS weight ratio of the product, first thoroughly mix the main paint with the precipitated zinc phosphate powder, then add the curing agent, mix and stir evenly
2. Maturity: Generally, let it stand for 10-30 minutes for pre reaction; Directly spraying without curing is prone to sagging, pinholes, and poor curing
3. Applicable period: mostly 4-8 hours at 20 ℃; the higher the temperature, the shorter the available time; Ready to use, do not mix too many at once, as they may become adhesive and scrapped after exceeding the time limit
4. Dilution: Only use the matching epoxy diluent, and do not add xylene or alcohol acid diluents casually; Airless spraying generally adds 5-15%, brush coating adds less, and excessive dilution will reduce rust prevention, sedimentation, and sagging
3、 Construction environmental conditions
Environmental temperature: 5-35 ℃. Curing is extremely slow below 5 ℃, and construction is not recommended; High temperature>35 ℃ is prone to dry spraying, orange peel peeling, and significantly shortened activation period
Relative humidity: ≤ 85%; Construction is strictly prohibited on rainy, foggy, and steel plate condensation days, as it may cause amine whitening (amine frost) and affect interlayer adhesion
Avoid construction in strong winds and exposed environments: The exposed steel plate heats up too high, and the solvent evaporates too quickly, which can easily cause pinholes and loss of gloss
4、 Film thickness and coating method
Conventional single pass dry film: 40-60 μ m; Too thick is prone to sagging and internal dryness; Too thin, insufficient rust prevention, poor coverage
Construction method: Prioritize airless spraying; Small area brushing/roller coating, edges, corners, and welds must be pre coated (strip coating), as edges and corners are prone to insufficient film thickness and early rusting
The wet film card can measure the wet film at any time and convert it to dry film; After completion, use a film thickness gauge for sampling inspection
5、 Repainting interval
Short interval: usually 6-10 hours at 20 ℃, must wait for the surface to dry and not stick to the hands before applying paint/intermediate coating
Maximum recoating window: usually 48-72 hours. If the maximum recoating time is exceeded, the epoxy surface will be completely cross-linked and smooth. It must be polished, brushed, and dust removed before recoating, otherwise interlayer delamination will occur
Supporting reminder: ✅ Can be equipped with epoxy intermediate coating, polyurethane topcoat, fluorocarbon topcoat; ❌ It is strictly prohibited to directly match with alkyd paint, as it may cause saponification, peeling, and detachment; It cannot be exposed to direct sunlight for a long time. It is only a primer and must be coated with a topcoat
6、 Drying, curing, and maintenance
Reference at 20 ℃: Dry for about 30-60 minutes on the surface, dry for about 6-9 hours on the surface; fully cured for 7 days, do not soak in water, salt spray, or heavy load friction for a long time within 7 days
If amine whitening occurs: lightly polish and then reapply; Serious adhesion failure, need to be removed and re sprayed
7、 Common Defects and Causes
Pinholes and bubbles: humidity too high, substrate with water, dilution too fast, spraying too thick
Poor adhesion: inadequate rust removal, uncleaned oil stains, failure to polish the maximum recoating interval, untreated galvanized sheet
Salt spray difference: insufficient film thickness, zinc phosphate precipitation not stirred evenly, too much diluent added, too little curing agent added
Flow hanging: excessive dilution, too thick spraying at once, too close spray gun distance
8、 Safety and Others
Forced ventilation in confined spaces, wearing gas masks and goggles; Keep away from open flames, it belongs to flammable solvent based coatings
Immediately clean the tool with the matching diluent after use, as the paint solidifies inside the gun and is difficult to clean
Store in a cool and sealed place. Zinc phosphate pigment is prone to precipitation, so be sure to stir thoroughly before opening the lid
Post time: Nov-25-2026